TYPICAL ABRASION RESISTANCE
Comparative taber abrasion resistance is shown to dramatize
the outstanding values obtained for polyurethane vs. other
polymers.
|
POLYMER
|
MG Weight Loss
|
| Polyurethane (aromatic
Polyester) |
3
|
| Polyester film
|
18
|
| Nylon 11 |
24
|
| High density
polyethylene |
29
|
| Polytetraflouroethlene
(PTFE) |
42
|
| Nitrile rubber
|
44
|
| Nylon 6/6 |
49
|
| Low density |
70
|
| High impact PVC
|
122
|
| Normal impact PVC
|
160
|
| Plasticized PVC
|
187
|
| Butyl rubber |
205
|
| ABS |
275
|
| Polychloroprene
|
280
|
| Polystyrene |
324
|
| Nylon 6 |
366
|
ASTM method D1044-CS-17 wheel with 1000g load, 5000 cycles